材料类型发光机理密度(g/cc)光产额(photons/MeV)衰减时间(ns)发射峰(nm)能量分辨率(% fwhm @ 662 keV)描述数据来源
(C6Hs(CH2)2NH3)2PbBr4SX2.5100009.4 + 200437vanEijk2008
(Gd-Y)3Al5O12:Ce (GYAG)Ce3+61100090 + >1,0005508ceramic; 0.5% CeYanagida2007
(Lu,Y)2SiO5:Ce (LYSO)Ce3+7.127000425Haas2008
AgGd(PO3)4:CeCe3+800014 ns (32%) + slow317; 333crystalline powder; 15% CeDerenzo2011
Al2O3Tl+2,300 (77K)138 (300K) + slow290 (30%); 420 (70%)0.2% Ti+Mikhailik2005
Al2O3:Ti3.982300290(33%); 730(67%)<150KMikhailik2007
AlO0.86N0.43Ce3+32 (alpha exc.)405transparent ceramicChen2015
Ba2B5O9Cl:EuEu2+11000640 (71%)420crystalline powder; 2% EuDerenzo2011
Ba2Ca(BO3)2:CeCe3+4.75100244007% Ce on Ba site + 7% NaLin2007
Ba2GdCl7:CeCe3+3000047(6%); 260 (11%); 1650 (20%) + slow355; 377crystalline powder; 10% CeDerenzo2011
Ba2MgSi2O7:EuEu2+10000280 ns (15%); 795 (80%)505crystalline powder; 2% EuDerenzo2011
Ba2P2O7:EuEu2+2500288 ns (19%); 632 (78%)421crystalline powder; 3% EuDerenzo2011
Ba2Si3O8:EuEu2+35000355 ns (10%); 1,400 (90%)505crystalline powder; 0.2% EuDerenzo2011
Ba2SiO4:EuEu2+40000242 ns (17%); 668 (81%)505crystalline powder; 0.2% EuDerenzo2011
Ba2SiO4:EuEu2+22000242; 668502; 525crystalline powder; 0.2% EuEagleman2012
Ba2YCl7:CeCe3+1500018 (80%)390; 414crystalline powder; 2% CeDerenzo2011
Ba2ZnSi2O7:EuEu2+16000665 ns (80%); 1,080 (18%)505crystalline powder; 1% EuDerenzo2011
Ba3(PO4)2:EuEu2+27000265 ns (23%); 620 (74%)420crystalline powder; 1.5% EuDerenzo2011
Ba3B(PO4)3:EuEu2+18000334 ns (13%); 820 (36%); 9,300 (39%)418crystalline powder; 2% EuDerenzo2011
Ba3Gd(BO3)3:CeCe3+5.3370313; 4184% CeHan2007
Ba3P4O13:EuEu2+25000288 ns (15%); 806 (83%)440crystalline powder; 2.5% EuDerenzo2011
Ba5(PO4)3F:CeCe3+4.76400358crystalline powder, 40% CeZeng2006
Ba5Si8O21:EuEu2+20000305 ns (17%); 852 (81%)453; 511crystalline powder; 1% EuDerenzo2011
BaAl10MgO17:EuEu2+16000315 ns (8%); 1,460 (74%)459crystalline powderDerenzo2011
BaAl12O19:EuEu2+50001,110 ns (36%); 15,000 (64%)433; 460crystalline powder; 0.5% EuDerenzo2011
BaBr1.7I0.3Eu2+112000329(23%); 640(40%)4145% Eu2+Gundiah2011
BaBr2SA4.7219,300 (10 us)2,200 + slow425; 4755.4Selling2007a
BaBr2:CeCe3+4.725,000 (0.5 us); 10,300 (10 us)80 (27%); 490 (22%); 2,100 (51%)345; 3709.81% Ce; 1% KSelling2007b
BaBr2:CeCe3+13,600 (10 us)1700100.1% Ce; Trise = 150 nsSelling2008
BaBr2:EuEu2+4.7215,700 (10 us)58540411Selling2007a
BaBr2:EuEu2+4.8558000267(21%); 655(55%)4145% Eu2+Gundiah2011
BaBr2:EuEu2+15,700 (10 us)585110.1% EuSelling2008
BaBr2:EuEu2+4.784900035 (8%); 415 (47%); 814 (44%)4086.95% EuYan2014
BaBrCl:EuEu2+4.559500285(14%); 546(56%)4055% EuGundiah2013
BaBrCl:EuEu2+4.5308004.255% EuYan2016
BaBrI:EuEu2+5.281000297(23%); 482(77%)4134.8Bourret2010
BaBrI:EuEu2+5.29700070 (1.5%); 432 (70%); 9,500 (28.5%)3.01 eV (42%); 2.91 eV (58%)3.48% Eu2+Bizarri2011
BaBrI:EuEu2+5.2189000313(59%); 741(15%)4135% Eu2+Gundiah2011
BaBrI:EuEu2+5.3710004804134.35% EuShirwadkar2013
BaCl2SA3.891,700 (10 us)980 + slow420; 47517.4Selling2007a
BaCl2SA3.8660001.6 (72%); 34.8 (28%)300-400Koshimizu2009
BaCl2:CeCe3+3.892,000 (0.5 us); 5,200 (10 us)7 (6%); 190 (11%); 1,500 (83%)349; 37316.21% Ce; 1% KSelling2007b
BaCl2:CeCe3+3.893,100 (10 us)14 (10%); 90 (40%); 1,400 (50%)140.1% CeSelling2008
BaCl2:EuEu2+3.8919,400 (10 us)3904028.8Selling2007a
BaCl2:EuEu2+3.8919,400 (10 us)3908.80.1% EuSelling2008
BaCl2:EuEu2+3.8952,000 (10 us)25 (15%); 138 (21%); 642 (61%)4063.55% EuYan2013
BaCl2:EuEu2+3.865200025 (15%); 138 (21%); 642 (61%)4063.55% EuYan2014
BaClBr:EuEu2+4.5520003.555% EuBourret2012
BaClI:EuEu2+4.65400095% EuBourret2012
BaF2SX4.8810000620310assumes 1 photoelectron per 5 photonsLaval1983
BaF2CV4.8820000.6220assumes 1 photoelectron per 5 photonsLaval1983
BaF2SX4.889950assumes 1 photoelectron per 5 photonsHoll1988
BaF2CV4.881300<1 ns2204.4% Ce; Luminosity 3% of NaI(Tl) with Bialkali PMTMelcher1989
BaF2SX4.883900340; 920310Luminosity 9% of NaI(Tl) with Bialkali PMTMelcher1989
BaF2CV4.8814000.8195; 2204.4% Ce; Luminosity 3% of NaI(Tl) with Bialkali PMTVanEijk1993
BaF2CV4.880.12 (15%); 0.78 (85%)Derenzo2000
BaF2SX4.881100011.4Sakai1987
BaF2:CeCe3+4.881300047; 2603200.2% Ce; luminosity 114% of undopedVisser1991
BaF2:CeCe3+4.88220050360Luminosity 5% of NaI(Tl) with Bialkali PMTMelcher1989
BaF2:CeCe3+4.884 (12%); 28 (78%)342-35835% CeGektin2009
BaFI:EuEu2+555000163 (7%); 573 (81%); 905 (6%)4058.55% EuGundiah2010
BaGdCl5:CeCe3+3500027 (11%); 87 (9%); 315 (17%); 1550 (19%)363; 389crystalline powder; 5% CeDerenzo2011
BaHfO3:CeCe3+8.34000025 + slow400transparent ceramicVanLoef2007
BaI2SA5.152,600 (0.5 us); 4,600 (10 us)590 (71%); 2,200 (29%)550Selling2007b
BaI2:CeSA5.152,600 (10 us)610 + slow5300.1% Ce but only slow SA emission detectedSelling2007a
BaI2:CeCe3+5.15not detected0.1% CeSelling2007a
BaI2:CeCe3+4,600 (10 us0590 (71%); 2,200 (29%)0.1% CeSelling2008
BaI2:EuEu2+5.153,800 (10 us)510 + slow425Selling2007a
BaI2:EuEu2+5.1>30,000< 1,000420Cherepy2008
BaI2:EuEu2+5.1400008Cherepy2009
BaI2:EuEu2+5.1322000317(36%); 646(42%)4265% Eu2+Gundiah2011
BaI2:EuEu2+3,800 (10 us)510 (32%) + slow0.1% EuSelling2008
BaI2:EuEu2+5.1538000513 (95%)4265.65% EuYan2014
BaKPO4:EuEu2+35000275 ns (31%); 645 (55%)425crystalline powder; 2% EuDerenzo2011
BaLu2F8CV6.944001+slow313VantSpijker1999a
BaLu2F8:CeCe3+6.9487035 + slow330VantSpijker1999a
BaMgF4CV4.51000190; 220VanEijk1993
BaP2O6:EuEu2+1900169 ns (38%); 795 (52%)380;470crystalline powder; 1% EuDerenzo2011
BaSi2O5;EuEu2+300002,800 ns (98%)520crystalline powder; 2% EuDerenzo2011
BaSiO3:EuEu2+8000170 ns (21%); 480 (30%); 1,300 (45%)510crystalline powder; 0.1% EuDerenzo2011
BaY2F8:CeCe3+4.9798046 + slow3299.9% Ce concentrationVantSpijker1999a
BC-408 (plastic)7500Salacka2010
BeOSX2.8665001825015% of NaI(Tl)Ogorodnikov1996
Bi4Ge3O12 (BGO)Bi3+7.138200Holl1988
Bi4Ge3O12 (BGO)Bi3+7.13300480Weber1973
Bi4Ge3O12 (BGO)Bi3+7.138080Mares2004
Bi4Ge3O12 (BGO)Bi3+7.138500Moszynski1997a
Bi4Ge3O12 (BGO)Bi3+7.13300485Grabmaier1984
Bi4Ge3O12 (BGO)Bi3+7.137610deHaas2005
Bi4Ge3O12 (BGO)Bi3+7.13106009.05Sakai1987
Bi4Ge3O12 (BGO)Bi3+7.1100 (12%) 300 (79%) 1000 (4%)460crystalline powderPorter2008
Bi4Ge3O12 (BGO)Bi3+7.137200510Haas2008
Bi4Ge3O12 (BGO)Bi3+7.137100luminosity = average of APD and PD valuesdehaas2008
Bi4Ge3O12 (BGO)Bi3+7.138000Salacka2010
Bi4Ge3O12 (BGO)Bi3+7.1320,000*7.2** -150C, 10 us peaking timeDerenzo1984
Bi4Si3O12 (BSO)Bi3+6.820001004803010,000 ph/Mev and 2,000 ns at 185KKobayashi1983
Bi4Si3O12 (BSO)Bi3+6.8105 ave 3.7 (7.5%); 28.8 (9.6%); 116.8 (87.5%)47024Harada2001
Bi4Si3O12:Ce (BSO)Bi3+6.81,200*86 ave 2.8 (7.4%); 27.1 (9.2%); 99.8 (83.4%)470290.1% Ce; *luminosity 60% of undopedHarada2001
BiBaO2BrBi3+6.712200100 (21%) 300 (54%) 700 (12%)500crystalline powder; luminosity 0.27 x BGOPorter2008
BiBaO2ClBi3+6.366600100 (2%) 300 (41%) 600 (23%)491crystalline powder; luminosity 0.81x BGOPorter2008
BiSrO2ClBi3+6.1200050 (28%) 200 (35%) 300 (14%)431crystalline powder; luminosity 0.24 x BGOPorter2008
Ca3Ga3Si2TaO14 (CTGS)SA120080(56%); 630(44%)34026Kurosawa2014
Ca4YO(BO3)3:CeCe3+110390; 420crystalline powderKnitel2000
Ca5(PO4)3F:CeCe3+3.23200354, 412crystalline powder, 2.5% CeZeng2006
CaBPO5:CeCe3+3.2131019.50.5% CePierron2003
CaBr2:EuEu2+3.353600025004489.15% EuGrippa2013a
CaF2:CeCe3+3.184 (3%); 14 (5%); 30 (92%)318; 33235% CeGektin2009
CaF2:EuEu2+3.1824000Holl1988
CaHfO3:CeCe3+1000033 ns (47%) + slow439crystalline powder; 1% CeDerenzo2011
CaI2SA3.9686000550410Hofstadter1964b
CaI2:EuEu2+3.9686000790470Hofstadter1964b
CaI2:EuEu2+3.961100008Cherepy2009
CaI2:TlTl+3.96420001100420Hofstadter1964b
CaLaB7O13:CeCe3+220291; 309; 330; 360crystalline powderKnitel2000
CaLaB7O13:EuEu2+not significantcrystalline powderKnitel2000
CaWO4CX6.115,000-25,0008000425Luminosity 90% of CdWO4Zdesenko2005
CaWO4CX6.11,400 (30%); 9,200 (70%)Mikhailik2007
CaWO4CX6.1158006.6Moszynski2005
CaWO4CX6.1144006.377KMoszynski2005
CaYBO4:EuEu2+not significantcrystalline powderKnitel2000
CdF2SX6.41707.1520;580Jones1962
CdF2SA6.611004.8 (29%); 24 (28%); 78 (43%)420crystalline powderDerenzo1990
CdS:InIn3+4.8<1519fast phosphorLehmann1966
CdS:InIn3+4.80.2520fast n-type phosphorDerenzo2005
CdS:In,TeIn3+, Te2- BT4.83.3630fast n-type phosphorDerenzo2005
CdS:TeTe2- BX4.817000270+slow640; 580Schotanus1992
CdWO4SA7.92700012000495Moszynski2005
CdWO4CX7.915300Holl1988
CdWO4CX7.978005,000; 20,000480Luminosity 18% of NaI(Tl) with Bialkali PMTMelcher1989
CdWO4CX7.98900480Grabmaier1984
CdWO4CX7.9122008Sakai1987
CdWO4CX7.915800130008.3300KKlamra2012
CdWO4CX7.9143408.877KKlamra2012
CeBr3Ce3+5.26800017371Shah2005
CeBr3Ce3+5800021360; 3803.21.9% Ca+Guss2014
CeBr3 + 1-propanolCe3+3218365Boatner2013
CeBr3 + isobutanolCe3+1920360Boatner2013
CeBr3 + tert-butanolCe3+309536012.6Boatner2013
CeCl3Ce3+3.94600025 + slow3503.4vanLoef2001b
CeCl3(CH3OH)4Ce3+1660064.4 (93%); 1,660 (7%)36411.4Boatner2008
CeF3Ce3+6.162400Wojtowicz1994
CeF3Ce3+6.1644003; 26.5Moses1990
CeF3Ce3+6.1640002; 31310; 340Anderson1989
CeF3Ce3+6.1640002734020Moses1989
CeF3:LuLu3+6.168000290Villora2005
CeP5O14Ce3+4000Wojtowicz1994
Cs2BaBr4:EuEu2+4.425,000 (est.)5% Eu2+Bourret2012
Cs2BaCl4:EuEu2+3.7530,000 (est.)5% Eu2+Bourret2012
Cs2BaI4:EuEu2+4.517,000 (est.)7% Eu2+Bourret2012
Cs2HfCl6CX3.86540004,370 (95%); 300 (5%)4003.3Burger2015
Cs2HfCl6SA275002,200; 8,400375; 435Saeki2016
Cs2HfCl6SA3.780.92 of NaI:Tl300 (5%); 4400 (95% )4003.3Burger2015
Cs2LiCeBr6Ce3+4.1828,000 (10 us)86(76%); 444 (8%); 3,800(16%)400; 4187.4Cheon2011
Cs2LiCeCl6Ce3+3.422000101(42%); 557(35%); 2,900(23%)385, 4055.5Rooh2010a
Cs2LiGdBr6:CeCe3+4.412500073 (63%); 542 (14%); 3,900 (23%)392; 4208.61% CeRooh2014a
Cs2LiGdBr6:CeCe3+4.413050039 (43%); 587 (31%); 1,100 (26%)392; 44310% CeRooh2014a
Cs2LiGdCl6:CeCe3+3.720000129 ns (51%); 573 ns (32%); 8.9 ms (17%)360; 460510% CeRooh2010c
Cs2LiLaBr6:Ce (CLLB)Ce3+4.26000041033.0 MeV gamma equivalentneutronGlodo2011
Cs2LiLaBr6:Ce (CLLB)Ce3+4.25000055; >270390; 4202.910% Ce3+Shirwadkar2011
Cs2LiLaCl6:Ce (CLLC)Ce3+350004003.43.1 MeV gamma equivalentneutronGlodo2011
Cs2LiLuCl6:CeCe3+3.9700029.4370; 4100.5% CeBessiere2006
Cs2LiLuI6:CeCe3+1100047 (30%); 220(32%); 1,400 (38%)435; 478100.5% Ce3+; 35,500 photons/neutronBirowosuto2008b
Cs2LiYBr6:CeCe3+4.152400085 (39%); 2,50071% Ce; 88,000 photons/neutronBessiere2004
Cs2LiYCl6SA3.316,535 (1 us); 22,420 (10 us)6600305Combes1999
Cs2LiYCl6CV3.316602250Bessiere2005a
Cs2LiYCl6SA3.317,000 (1us); 22,00 (10 us)7000Bessiere2005a
Cs2LiYCl6CV3.3117004Bessiere2004
Cs2LiYCl6:Ce (CLYC)Ce3+3.319,565 (1 us); 18,400 (10 us)600; 6,000372; 400Combes1999
Cs2LiYCl6:Ce (CLYC)Ce3+3.312100035 + slow49060.5% CevanLoef2005b
Cs2LiYCl6:Ce (CLYC)Ce3+3.3110,200 (1us); 21,600 (10 us)28003700.1% CeBessiere2005a
Cs2LiYCl6:Ce (CLYC)Ce3+3.312160080.1% Ce; 70,000 photons/neutronBessiere2004
Cs2LiYCl6:Ce (CLYC)Ce3+3.35.1>1% Ce; neutron peak resolution 2.9%Glodo2008a
Cs2LiYCl6:Ce (CLYC)Ce3+200003904.53.5 MeV gamma equivalentneutronGlodo2011
Cs2LiYCl6:PrPr3+3.3110000315150.2% PrvanLoef2005b
Cs2NaCeBr6Ce3+425000140 us (94%); 880 us (6%)380-4666.7Kim2009a
Cs2NaCeBr6Ce3+4.2525000140(94%); 800(6%)377, 4006.7Kim2010
Cs2NaCeCl6Ce3+Rooh2009
Cs2NaGdBr6:CeCe3+4.183680072 (67%); 266 (22%); 698 (11%)393; 4225.110% CeRooh2012
Cs2NaGdBr6:CeCe3+4.194800065 (48%); 193 (24%); 864 (8%); >6,000 (20%)389; 4183.34% Ce3+Samulon2014
Cs2NaGdCl6:CeCe3+3.52100069 ns (34%); 503 ns (37%); 3,200 (29%)378; 400 nm0.04810% Ce3+Rooh2014
Cs2NaGdCl6:CeCe3+3.5227000110 (15%); 353 (18%); 1,572 (24%);>6,000 (44%)375; 40342% Ce3+Samulon2014
Cs2NaLaBr6:CeCe3+9,000 (0.5 us); 17,000 (10 us)61 (32%) 450 (11%) 1,900 (57%)382; 41411.30.5% CeBirowosuto2006d
Cs2NaLaBr6:CeCe3+3.934600048(18%); 205(21%); 854(23%); 4021(36%)385; 4133.94% Ce; 11 ns rise timeGundiah2014
Cs2NaLaCl6:CeCe3+3.262640066(18%); 340(18%); 1620(45%)373; 4054.44% Ce; 16 ns rise timeGundiah2014
Cs2NaLuBr6:CeCe3+5,200 (0.5 us); 5,800 (10 us)61 (65%) 350 (35%)389; 42210.50.5% CeBirowosuto2006d
Cs2NaLuCl6:CeCe3+1(1%); 55 (44%); 380(55%)Birowosuto2009
Cs2NaLuI6:CeCe3+30(100%)Birowosuto2009
Cs2NaYBr6:CeCe3+5,000 (0.5 us); 9,500 (10 us)61 (26%) 350 (23%) 2,700 (51%)385; 4206.30.3% CeBirowosuto2006d
Cs2ZnCl4CV3.356301.8 (95%); 10255; 280; 390Yahaba2014
Cs2ZrCl6SA251001,500; 7,500440; 479Saeki2016
Cs3CeCl6Ce3+3.41900050 (50%); 300 (50%)4008.4Zhuravleva2011
Cs3Gd2I9:CeCe3+4.732,200 (0.5 us); 2,600 (10 us)1% CeBirowosuto2007b
Cs3GdBr6:CeCe3+4.144700072 (26%); 270 (25%); 1,421 (26%); >6,000 (23%)396; 42544-8% Ce3+Samulon2014
Cs3GdCl6:CeCe3+3.562450039 (7%); 129 (12%); 462 (15%); 2,110 (36%); >6,000 (30%)382; 4074.58% Ce3+Samulon2014
Cs3LaBr6SA4.551,600 (0.5 us); 2,100 (10 us)250 (92%) 2,100 (8%)39413.6Birowosuto2007b
Cs3LaBr6:CeCe3+4.555,800 (0.5 us); 10,400 (10 us)46 (18%) 270 (42%) 2,100 (40%)390; 425300.5% CeBirowosuto2007b
Cs3LaBr6:CeCe3+3.993500071 (72%); 437 (28%)410810% CeWei2014
Cs3LaBr6:CeCe3+3.823250044(17%); 1214(18%); 399(20%); 2230(31%)393; 4254.915% Ce; <0.1 ns rise timeGundiah2014
Cs3LaCl6:CeCe3+3.272000056 (75%); 380 (25%)400920% CeWei2014
Cs3LaCl6:CeCe3+3.361600079(32%); 291(33%); 1243(28%)383; 4158.68% Ce; 13 ns rise timeGundiah2014
Cs3Lu2I9SA4.824,000 (0.5 us); 6,600 (10 us)770390; 60819.2Birowosuto2007b
Cs3Lu2I9:CeCe3+4.8213,600 (0.5 us; 22,800 (10 us)18 (2%); 42 (6%) 120 (40%); 510 (52%)92% CeBirowosuto2007b
Cs3LuI6SA4.781,200 (0.5 us); 1,400 (10 us)390; 608Birowosuto2007b
Cs3LuI6:CeCe3+4.781,400 (0.5 us); 1,500 (10 us)429; 4710.5% CeBirowosuto2007b
CsBa2Br5:EuEu2+4.550,000 (est.)2% EuBourret2012
CsBa2Br5:EuEu2+4.4892000378 (6%); 1260 (67%)4352% Eu2+Borade2011
CsBa2I5:EuEu2+59700048 (1%); 383 (26%); 1,500 (68%); 9,900 (25%)4353.87% EuBourret2009a
CsBa2I5:EuEu2+4.9102000384 (10%); 1,200 (58%); 14,000 (32%)2.85 eV (45%); 2.7 eV (19%); 2.66 eV (36%)2.554% EuBizarri2011
CsBa2I5:EuEu2+5800009004303.93% EuShirwadkar2013
CsBa2I5:EuEu2+4.9800003504340.0235% EuAlekhin2014
CsBa2I5:InIn3+4.53500032(2%); 162(8%); 1980(43%)5407.10.2% InGascon2014
CsBa2I5:NaNa+4.53350039(7%); 183(36%); 995(37%)4307.91.0% NaGascon2014
CsBa2I5:TlTl+4.54000028(1%); 414(42%); 1241(24%)5007.10.08% TlGascon2014
CsBa2I5:YbYb2+4.9540008704145.71% Yb2+Rowe2013
CsBrCV4.4200.07250VanEijk1993
CsCaBr3:EuEu2+28000145(0.43%); 6,097(89.8%); 28,000(9.8%)4479.38% EuGrippa2013b
CsCaCl3CV2.91400< 1250; 305VanEijk1993
CsCaCl3:EuEu2+31800050504508.9Zhuravleva2012
CsCaI3:EuEu2+4.063850017204508Zhuravleva2012
CsCaI3:EuEu2+30,000-22,000 (size dependent)2100-3900 (size dependent)4554.5 - 13 (size dependent)3%Eu in meltLindsey2015a
CsCe2Br7:CeCe3+43556278 (52.0%); 316 (31.6%); 1723(16.4%)390; 420; 4757Wu2015
CsCe2Cl7Ce3+3.62600050 (52%); 210 (47%)3857.5Zhuravleva2011
CsCe2Cl7:CeCe3+3.61947066 (87.3%); 351 (12.7%)12Wu2015
CsClCV49000.9240; 270VanEijk1993
CsFCV4.64190044961390Moszynski1983
CsFCV4.120002.9390VanEijk1993
CsGd(PO3)4:CeCe3+4.0724400336, 358crystalline powder; 1% CeZhong2009
CsGd2F7:CeCe3+5.5730020 + 3,00032520% CeSchaart1995
CsGd2F7:CeCe3+5.56000~30 (18%) + 3,00034013.510% CeDorenbos1993
CsGd2F7:PrPr3+5.5d-f not observed2% PrDorenbos1993
CsISX4.5116.7Sakai1987
CsI:CO3SA4.51390001760410; 5008.350.1% CO3Ha2009
CsI:EuEu2+4.5119100Holl1988
CsI:InIn+4.5127,000 (12 us)19005459.5Gridin2013
CsI:NaNa+4.5138000Holl1988
CsI:NaNa+4.5149000deHaas2005
CsI:NaNa+4.51430007.4Sakai1987
CsI:NaNa+4.5149000425Haas2008
CsI:NaNa+4.5146000luminosity = average of APD and PD valuesdehaas2008
CsI:TlTl+4.5155000Holl1988
CsI:TlTl+4.5161000Moszynski1997a
CsI:TlTl+4.51980530Grabmaier1984
CsI:TlTl+4.5156000deHaas2005
CsI:TlTl+4.51560005.7Sakai1987
CsI:TlTl+4.5157000560Haas2008
CsI:TlTl+4.5156000luminosity = average of APD and PD valuesdehaas2008
CsLuP2O7:CeCe3+4.4980004.4 (14.1%); 19.8(85.9%)393crystalline powder; 0.5% CeYuan2007
CsSrBr3:EuEu2+3.840,000 (est.)3% Eu2+Bourret2012
CsSrBr3:EuEu2+31300250044295% EuCherginets2014
CsSrCl3:CeCe3+86003.8 (23%); 57 (23%); 626 (54%)360-3857.20.5% CeFujimoto2017a
CsSrCl3:EuEu2+33400270044811.55% EuCherginets2014
CsSrI3:EuEu2+650005.98% Eu2+Yang2011
CsY2F7:CeCe3+1400323335% CeSchaart1995
CsYP2O7:CeCe3+3.5780005.2 (16.9%); 22.2(83.1%)393crystalline powder; 0.5% CeYuan2007
Ga2O3SA150008; 977380Yanagida2016
Gd2Si2O7:Ce (GPS)Ce3+5.530,000-40,00046372; 3946luminosity 2.5 x GSO, 5 x BGOKawamura2007
Gd2SiO5:Ce (GSO)Ce3+6.711250056; 6004307Melcher1996
Gd2SiO5:Ce (GSO)Ce3+6.7128007.8Sakai1987
Gd2SiO5:Ce (GSO)Ce3+6.7174009.2Balcerzyk2000b
Gd3Al2Ga3O12:CeCe3+4221752.8(73%); 282(27%survey of 23 members of (Lu,Gd)3 (Ga,Al)5 O12:Ce familyKamada2011
Gd3Al3Ga2O12:CeCe3+45931221 (100%)survey of 23 members of (Lu,Gd)3 (Ga,Al)5 O12:Ce familyKamada2011
Gd3Sc2Al3O12:Ce (GSAG)Ce3+750010.8ceramic, 3% CeCherepy2009
Gd3Y3Al10O24:Ce (GYAG)Ce3+1650011.2ceramic, 3% CeCherepy2009
GdAlO3:CeCe3+7.5900030; 180335; 3580.75% CeDorenbos1995b
GdB3O6:CeGd3+200311crystalline powder; Ce3+ to Gd3+ transferKnitel2000
GdBO3:CeCe3+6.310000385; 415crystalline powderKnitel2000
GdBr3Ce3+4.5528,000 (0.5 us); 44,000 (10 us)20 (26%) 212 (65%) 13,500 (9%)4602% CevanLoef2001a
GdCl3:CeCe3+4.5438000350; 3701% CeGrippa2010
GdI3:CeCe3+5.289000335632% CeGlodo2008
GdI3:CeCe3+5.24400045 (70%); 250 (24%); 2,000 (6%)5604.71% Ce; 42,000 ph/MeV at 600 KBirowosuto2008a
GdNb0.2Ta0.8O4SA8.37260012(100%)450luminosity 13 x PbWO4Voloshyna2014
GdOBr:CeCe3+89% of ZnS:Ag60405, 440phosphor, 1% CeBuchanan1981
GdOBr:CeCe3+6.8234,000*30 (100%); 10 risetime405; 445* 0.49 x LaBr3:Ce; crystalline powderEagleman2011
GdOCl:CeCe3+75% of ZnS:Ag36365, 410phosphor, 1% CeBuchanan1981
GdOCl:CeCe3+6.6617,000*25 (63%); 76 (27%); 6 risetime400* 0.25 x LaBr3:Ce; crystalline powder; 0.5% CeEagleman2011
GdOF:CeCe3+7.69not observedcrystalline powderEagleman2011
GdOI:CeCe3+6.857,000*23 (67%)440; 470* 0.10 x LaBr3:Ce; crystalline powder; 2% CeEagleman2011
HfF4SA7.130029350crystalline powderDerenzo1990
HfO2SA9.68310009.5480crystalline powder; 2.5% Eu, 1% YLeLuyer2008
K2BaI4:EuEu2+63000720 (67%); 3,100 (33%)4482.97% Eu2+Stand2016
K2CeBr5Ce3+2.9500006.310% CeHawrami2008
K2CeCl5Ce3+2.9300003705.8Roy2007
K2LaBr5:CeCe3+3.940,000 (10 us)50359; 39110% CevanLoef2005
K2LaCl5SX2.89900370040010% CeVantSpijker1999b
K2LaCl5:CeCe3+2.8949,300; 22,600 (0.5 us)80 + slow347; 37210% CeVantSpijker1999b
K2LaCl5:CeCe3+2.923,000 (0.5 us); 30,000 (10 us)344; 37210% CevanLoef2005
K2LaI5:CeCe3+4.453,000 (0.5 us); 55,000 (10 us)24401; 43910% CevanLoef2005
K2LaI5:CeCe3+4.429000340; 3805.110% Ce; 50% in 115 nsvantSpijker1995
K2LiYBr6:CeCe3+1040030 (1%); 250 (30%); 1,900 (69%)385; 420221% Ce3+: 37,000 photons/neutronBirowosuto2008b
K2YF5CV3.63001.3170VanEijk1993
K2YF5:PrPr3+3.16.920 (5%); + slow2402% PrDorenbos1993
K3Lu(PO4)2:CeCe3+3.92650034 (81%); 1200 (19%)390171% CeWisniewski2004
KBa2I5:EuEu2+4.5290000910 (81%); 4,900 (19%)4442.44% Eu2+Stand2016
KCaF3CV31400< 2140-190VanEijk1993
KCaI3:EuEu2+3.8172000106046533% Eu2+Lindsey2015
KGd(PO3)4:CeCe3+3.5214100325, 345crystalline powder; 1% CeZhong2009
KI:TlTl+3.19700Holl1988
KLu2F7CV7,5270< 2165VanEijk1993
KLuF4CV5.21701.3170-200VanEijk1993
KLuP2O7:CeCe3+3.87160006.3 (14.9%); 27.2(85.1%)394crystalline powder; 0.5% CeYuan2007
KMgF3CV3.214001.3140-190VanEijk1993
KSr2Br5:EuEu2+3.987500010764273.55% Eu2+Stand2015a
KSr2I5:EuEu2+4.39940009904452.44% Eu2+Stand2015b
KSr2I5:EuEu2+4.3994000990 (89%); 5,000 (11%)4522.4Stand2013
KSr2I5:EuEu2+4.39953008904452.84% Eu2+Stand2016
KYF4CV3.610001.9170VanEijk1993
KYP2O7:CeCe3+3.11100006.7 (22.6%); 23.2(77.4%)380crystalline powder; 0.5% CeYuan2007
La2Hf2O7:TiTi4+7.91300010000475transparent ceramic; 2% Ti4+Ji2005
La2O2S:CeCe3+5.82Not detectedYen1996
La2O3:CeCe3+6.6Not detectedYen1996
La2O3:CeCe3+6.6Not detectedvanderKolk2007
LaAlO3:CeCe3+6.5Not detectedvanderKolk2007
LaB3O6:CeCe3+4.27700300; 320crystalline powder; 0.05% CeKnitel2000
LaBO3:BiBi3+5.2800365Blasse1968
LaBO3:CeCe3+5.2600355; 380crystalline powderKnitel2000
LaBr(3-x)I(x):CeCe3+5.4742,000(0.5 us); 45,000(10 us)31(70%); 244(30%)400; 4344.1all entries for x = 0.75 and 5% CeBirowosuto2008
LaBr(3-x)I(x):CeCe3+5.5155,000(0.5 us); 58,000(10 us)28472; 50014.6all entries for x = 1.5 and 5% CeBirowosuto2008
LaBr(3-x)I(x):CeCe3+5.622,000(0.5us); 22,000(10 us)12460; 51035.9all entries for x = 2.25 and 5% CeBirowosuto2008
LaBr2:PrPr3+5.174500110003.21% Pr3Glodo2006
LaBr3:CeCe3+5.16100030356; 3872.90.5% CevanLoef2002
LaBr3:CeCe3+5.1730002.7-3.2sizes 5-76 mm; 5% CeMenge2007
LaBr3:CeCe3+5.17400037510% CeHaas2008
LaBr3:CeCe3+5.1750005% Ce; luminosity = average of APD and PD valuesdehaas2008
LaBr3:CeCe3+5.168600Salacka2010
LaBr3:CeCe3+5.178000~17 + slower2Sr2+ and Ca2+ co-dopingAlekhin2013
LaBr3:CeCe3+5.1rise time 9 ns ; decay time 26 ns0.5% Ce3+Glodo2005a
LaBr3:CeCe3+5.1rise time 0.2 ns ; decay time 17 ns20% Ce3+Glodo2005a
LaBr3:CeCe3+5.164000165% CeBizarri2007
LaBr3:CeCe3+5.156000300.2% CeBizarri2007
LaBr3:CeCe3+5.126 (9 ns rise time)0.5% CeGlodo2004
LaBr3:CeCe3+5.117 (<0.5 ns rise time)5% CeGlodo2004
LaCeF6Ce3+4500Wojtowicz1994
LaCl3SX3.8340003480400vanLoef2001b
LaCl3:CeCe3+3.84900025 + slow330; 3523.110% CevanLoef2001b
LaCl3:CeCe3+3.8480003505% CeHaas2008
LaCl3:CeCe3+3.85000010% Ce; luminosity = average of APD and PD valuesdehaas2008
LaCl3:CeCe3+3.840900Salacka2010
LaF3:CeCe3+5.922003; 26.5290; 34010% CeMoses1990
LaF3:NdNd3+5.9420006.31730.03% NdSchotanus1988
LaF3:NdNd3+5.9427017310.6% NdDorenbos1996
LaI3:CeCe3+5.6200-30044928452; 502luminosity 16,000 photons/MeV at 100KBessiere2005b
LaMgB5O10:CeCe3+1300310; 317crystalline powder; 0.05% CeKnitel2000
LaNb5O14SA7503,000 (73%)445crystalline powderDerenzo2011
LaNbO4SA110002,900 (71%)436crystalline powderDerenzo2011
LaOBr:CeCe3+38% of ZnS:Ag38460phosphor, 1% CeBuchanan1981
LaOBr:CeCe3+6.173,000*1 (11%); 4 (26%); 13 (35%)425* 0.04 x LaBr3:Ce; crystalline powderEagleman2011
LaOCl:BiBi3+1600345Blasse1968
LaOCl:CeCe3+4.3% of ZnS:Ag100435phosphor, 1% CeBuchanan1981
LaOCl:CeCe3+5.45<700*17 (15%); 106 (16%); 836 (15%)420* <0.01 x LaBr3:Ce; crystalline powder; 2% CeEagleman2011
LaOF:CeCe3+6.03not observedcrystalline powderEagleman2011
LaOI:CeCe3+5.917,500*24 (86%)470* 0.11 x LaBr3:Ce; crystalline powderEagleman2011
LaSCl:CeCe3+6505.5 ns (11%); 25 (51%); 102 (28%)460crystalline powder; 10% CeDerenzo2011
LaScO3:CeCe3+9002.2 ns (63%); 7.3 (19%)444crystalline powder; 1% CeDerenzo2011
Li12LuGd(BO3)6Ce3+60(28%); 313(14%); 30,000 (58%)4000.19Fawad2014
Li2CaSiO4:CeCe3+2.97800270.5% CePierron2003
Li2NaYBr6:CeCe3+1240030 (3%); 560 (11%); 2,600 (86%)383; 413101% Ce3+: 37,000 photons/neutronBirowosuto2008b
Li3TaO4SA300006,100 (67%)398crystalline powderDerenzo2011
Li3YCl6:CeCe3+2.453305 (1 us); 6185 (10 us)250; 2,300360; 385Combes1999
Li6Gd(BO3)3:CeCe3+14000385; 415crystalline powderKnitel2000
Li6Y(BO3)3:CeCe3+1200388; 419crystalline powderKnitel2000
LiBaF3CV5.214000.8190; 230VanEijk1993
LiBaF3SX5.2416006000300Knitel1996
LiBaF3CV5.2412000.8187; 225Knitel1996
LiCa2I5Eu2+900001416 (gamma exc.); 156 1370 (neutron)4725.6Soundara-Pandian2016
LiCaAlF6:CeCe3+3502806 ns rise timeGetkin2003
LiCaPO4:CeCe3+2.9590025.50.5% CePierron2003
LiGd(PO3)4:CeCe3+3.542600310, 329crystalline powder; 1% CeZhong2009
LiGdCl43.736000310; 340; 360crystalline powderPorter2009
LiGdCl4:CeCe3+3.76460033345; 365crystalline powder; 20 % CePorter2009
LiI:EuEu2+4.08150004757.5Syntfeld2005
LiI:EuEu2+4.081200Murray1958
LiInSe2440031(49%); 143(51%)yellow crystal formWiggins2015
LiInSe2not observedred crystal formWiggins2015
LiLuF4:CeCe3+3600320310; 335Yanagida2011
LiSr2Br5Eu2+320001418 (gamma exc.); 1261 (neutron)407; 4766.1Soundara-Pandian2016
LiSr2I5Eu2+600001330 (gamma exc.); 1262 (neutron)493; 417 (size dependent)3.53% EuSoundara-Pandian2016
LiYSiO4:BiBi3+350Blasse1968
Lu(2-2x)Gd(2x)SiO5:Ce (LGSO)Ce3+2000012.4x = 0.037 in crystalBalcerzyk2000b
Lu(x)Gd(1-x)I3:CeCe3+7840029540x= 0.7; 2% CeGlodo2008
Lu(x)Y(1-x)I3:CeCe3+6810028522x= 0.7; 2% CeGlodo2008
Lu1.8Y0.2SiO5:Ce (LYSO)Ce3+7.13400041 + slow397Pidol2004
Lu2.25Y0.75Al5O12:PrPr3+6.2330004.4Drozdowski2014
Lu2O3:CeCe3+9.52Not detectedYen1996
Lu2O3:CeCe3+9.5Not detectedvanderKolk2007
Lu2S3:CeCe3+6.252800032592VantSpijker1998
Lu2Si2O7:Ce (LPS)Ce3+6.22300030380Pauwels2000
Lu2Si2O7:Ce (LPS)Ce3+6.22600038378Pidol2004
Lu2Si2O7:Ce (LPS)Ce3+6.296000.25% CeCutler2009
Lu2SiO5:CeCe3+7.428000luminosity = average of APD and PD valuesdehaas2008
Lu2SiO5:Ce (LSO)Ce3+7.43300040420Melcher1992
Lu2SiO5:Ce (LSO)Ce3+7.427300Moszynski1997a
Lu2SiO5:Ce (LSO)Ce3+7.427000404207.9Melcher1996
Lu2SiO5:Ce (LSO)Ce3+7.47 (1%); 38.8 (99%)risetime: < 50 ps (88%); 350 ps (12%)Derenzo2000
Lu2SiO5:Ce (LSO)Ce3+7.429000425Haas2008
Lu2SiO5:Ce (LSO)Ce3+7.4260008.4Balcerzyk2000b
Lu2SiO5:Ce (LSO)Ce3+7.4222000.02% CeCutler2009
Lu2SiO5:Ce,CaCe3+7.43880036.74207.70.1% Ce3+, 0.1% Ca2+Spurrier2008
Lu2SiO5:Ce/Ca (LSO)Ce3+7.4254000.1% Ce; 0.1% CaCutler2009
Lu2SiO5:PrPr3+7.42,200 + slow26247Nikl2006
Lu2SiO5:Pr,CaPr3+7.46.9 (66%); 23.2 (34%) + slow0.2% Pr3+, 0.1% CaYang2009
Lu3Al5O12:Ce (LuAG)Ce3+6.712500Mares2004
Lu3Al5O12:Ce (LuAG)Ce3+6.75606510Lempicki1995
Lu3Al5O12:PrPr3+6.717000213100.14 % PrOgino2006
Lu3Al5O12:PrPr3+6.716000263080.25% PrNikl2005
Lu3Al5O12:PrPr3+6.72000020 (68%); 455 (32%)0.25% PrOgino2006a
Lu3Al5O12:PrPr3+6.71600017.2 (30%); 53 (16%); 1,590 (54%)3105Swiderski2009
Lu3Al5O12:PrPr3+6.7124001% PrCutler2009
Lu3Al5O12:PrPr3+6.719000203104.6Drozdowski2008
LuAlO3:Ce (LuAP)Ce3+8.341140016.5; 743650.105% CeMoszynski1997b
LuAlO3:Ce (LuAP)Ce3+8.36960011; 28; 835390Moses1995
LuAlO3:Ce (LuAP)Ce3+8.3411300Moszynski1997a
LuAlO3:Ce (LuAP)Ce3+8.342050017.9365Lempicki1995
LuBO3:Ce (Calcite)Ce3+6.810,800 (0.5 us); 12,000 (10 us)5% CeZhang1999
LuBO3:Ce (vaderite)Ce3+7.43,000 (0.5 us); 3,900 (10 us)5% CeZhang1999
LuBO3:Pr (Calcite)Pr3+6.84,200 (0.5 us); 7,300 (10 us)1% PrZhang1999
LuBO3:Pr (vaderite)Pr3+7.44,200 (0.5 us); 7,300 (10 us)1% PrZhang1999
LuBr3:CeCe3+5.22600032 + slow0.76% CevanLoef2003
LuCl3:CeCe3+4660046 + slow0.45% CevanLoef2003
LuF3:CeCe3+8.3800028310Birowosuto2009
LuI3:CeCe3+5.65000031 (69%); 400 (15%); 3,000 (16%) + slow475; 520Glodo2005
LuI3:CeCe3+5.65000023-31474decay time depends on Ce3+ concentrationShah2004
LuI3:CeCe3+5.676,000 (0.5 us; 98,000 (10 us)complex5405% CeBirowosuto2006a
LuI3:CeCe3+5.6876,000 (0.5 us; 98,000 (10 us)complex5403.35% CeBirowosuto2006c
LuI3:CeCe3+5.6115000285222% CeGlodo2008
LuOBr:CeCe3+7.6403, 432Rabatin1982
LuOBr:CeCe3+7.587,000*25 (56%); 73 (10%)405; 445* 0.10 x LaBr3:Ce; crystalline powder; 0.5% CeEagleman2011
LuOCl:CeCe3+7.2weak x-ray luminescence reportedRabatin1982
LuOCl:CeCe3+7.165,500*377 (16%); 1,512 (77%)380* 0.08 x LaBr3:Ce; crystalline powder; 0.5% CeEagleman2011
LuOF:CeCe3+not observedcrystalline powderEagleman2011
LuOI:CeCe3+7.71700*23 (82%); 73 (10%)430; 480* 0.01 x LaBr3:Ce; crystalline powder; 1% CeEagleman2011
LuPO4:CeCe3+6.531720025360Lempicki1993
LuScBO3:CeCe3+420031370Yanagida2011
MgSr2Si2O7:EuEu2+4000186 ns (50%); 435 (31%)465crystalline powder; 2% EuDerenzo2011
Na2Gd2B2O7:CeCe3+600036 ns (50%); 66 (42%)447; 478crystalline powder; 2 % CeDerenzo2011
NaBaPO4:EuEu2+20000355 ns (32%); 885 (64%)450; 610crystalline powder; 0.5% EuDerenzo2011
NaGd(PO3)4:CeCe3+3.622100012.4313; 332crystalline powder, 2.5% CeZhong2007
NaGd(PO3)4:CeCe3+3.6211100314, 333crystalline powder; 1% CeZhong2009
NaGdCl43.442400305; 345; 365crystalline powderPorter2009
NaGdCl4:CeCe3+3.443940026350; 370crystalline powder; 20% CePorter2009
NaI(pure)SX3.678000060 ns77K, 14% FWHM for 122 keV gammasPersyk1980
NaI(pure)SX3.673.877K, 50,000 ns peaking timeMoszynski2008
NaI:TlTl+3.67450004157.1Sakai1987
NaI:TlTl+3.6743000Holl1988
NaI:TlTl+3.67415Grabmaier1984
NaI:TlTl+3.675.6Persyk1978
NaI:TlTl+3.6744000415Haas2008
NaI:TlTl+3.6745000luminosity = average of APD and PD valuesdehaas2008
NaI:Tl, EuTl+, Eu2+3.67440006.3Shiran2010
NaI:Tl, Eu, CaTl+, Eu2+3.67520004.90.1% Tl+, 0.1% Eu2+, 0.2% Ca2+Khodyuk2015
NaI:Tl,Caco-doping Tl, Ca34,000 ± 1,800173 ± 12 (94%); 830 ± 230 (6%)4185.40.03±0.01%Tl 0.21±0.03%Ca (at. % in the melt, with respect to Na+) Improved non-proportionalityYang2015
NaI:Tl,Srco-doping Tl, Sr26,000 ± 3,100172±10 (92%); 860±160 (8%)4145.30.05±0.02%Tl 0.11±0.01%Sr (at. % in the melt, with respect to Na+) Improved non-proportionalityYang2015
NaLaSiO4:CeCe3+500026 ns (32%) + slow405crystalline powder; 5% CeDerenzo2011
NaLuP2O7:CeCe3+4.1160005.5 (17.7%); 20.4(82.3%)370crystalline powder; 0.5% CeYuan2007
PbCl2Pb2+5.92302.9 (41%); 20 (32%); 179 (27%)500crystalline powderDerenzo1990
PbCl2:GdGd3+5.91,350; 6,20025.60.1% Gd; 173KKim2008
PbCO3Pb2+6.67605.6; 27; 155475Luminosity 16,000 photons/MeV at -40CMoses1990
PbCO3Pb2+6.66802.0 (22%); 15 (69%); 92 (9%)432; 46511,900 photons/MeV at -120CMoses1991
PbFClPb2+7.1117004; 35392; 420Chen2004
PbFClK+7.11360550Yang2014
PbI2d-a6.164000010% in first ns52014K; native defect donor-acceptor recombinationDerenzo2013
PbSO4Pb2+6.449001.8; 19; 95; 425335Luminosity 68,500 photons/MeV at -145CMoses1992
PbSO4Pb2+6.4100001.85; 14.5; 125-150340; 380Zadneprovski2004
PbSO4Pb2+6.47.2 (21%); 35 (32%); 104 (39%); 656 (5.5%)35Zhang1994
PbWO4CX8.282006420QRTAnnenkov2002
PbWO4CX8.23002.5 (25%); 11 (29%); 98 (46%)490crystalline powderDerenzo1990
PbWO4:PrPr3+8.22502000480, 620, 6401% PrNikl2008
Polyvinylcarbazole (PVK) + diphenylanthracene (DPA) + bismuth tryphenylorganic12000154209PVK with DPA fluor loaded with 40% bismuth triphenyl by weightRupert2012
Polyvinylcarbazole (PVK) + diphenylanthracene (DPA) + bismuth tryphenylorganic30000120005007PVK with Ir-complexes fluor loaded with 40% bismuth triphenyl by weightRupert2012
PrBr3:CeCe3+5.3210008 + 22365; 39520% CeBirowosuto2006b
PrF3Pr3+6.3510394Villora2005
Rb2CeBr5Ce3+4.263400056.1 (98.8%); 329.9 (1.2%)390.56.9Kim2009
Rb2LiCeBr6Ce3+4.63300055 (87%); 284 (13%)3906.3Rooh2010b
Rb2LiCeCl6Ce3+3.12310071 (85%); 405 (15%)3707.9Rooh2012
Rb2LiLaBr6:CeCe3+3300026 (5%); 310 (37%); 1,100 (58%)363; 3874.81% Ce3+: 54,000 photons/neutronBirowosuto2008b
Rb2LiYBr6:CeCe3+3.822300042 (3%); 140 (23%); 1,600 (74%)385; 4204.70.5% CeBirowosuto2007a
Rb2LiYBr6:CeCe3+2300042 (3%); 140 (23%); 1,600 (74%)381; 4144.70.5% Ce3+; 83,000 photons/neutronBirowosuto2008b
Rb2LiYI6:CeCe3+71(53%); 400(31%); 1,400 (16%)Birowosuto2009
Rb2LiYI6:CeCe3+1100071 (31%); 400 53%); 1,400 (16%)435; 480280.5% Ce3+; 37,000 photons/neutronBirowosuto2008b
RbClCV2.81190VanEijk1993
RbFCV3.617001.3203; 234VanEijk1993
RbGd2Br7:CeCe3+4.85600045430Shah2002
RbGd2Br7:CeCe3+4.856000434104.19.8% CeGuillotNoel1999b
RbGd2Br7:CeCe3+4.755000604203.85% Ce3+Dorenbos1997
RbLuP2O7:CeCe3+4.213006.3 (23.2%); 24.0(76.8%)393crystalline powder; 0.5% CeYuan2007
RbYP2O7:CeCe3+3.2770008.8 (14.8%); 27.8(85.2%)393crystalline powder; 0.5% CeYuan2007
Sc2O3SA3.83770038; 21735022crystalFukabori2012
ScBO3:BiBi3+3.5300Blasse1968
ScBO3:CeCe3+3.56500385; 420crystalline powderKnitel2000
Sr5(PO4)3F:CeCe3+4.17340342crystalline powder, 25% CeZeng2006
SrAl2O4:CeCe3+3900303801% Ce3+Nakauchi2016
SrBr2:EuEu2+4.25250008Cherepy2009
SrBrI:EuEu2+4.947,000 (est.)5% Eu2+Bourret2012
SrClI:EuEu2+4.170,000 (est.)5% Eu2+Bourret2012
SrF2:CeCe3+4.34 (24%); 30 (76%)340-35035% CeGektin2009
SrHfO3:CeCe3+6.74000042 + slow410transparent ceramicVanLoef2007
SrI2SA4.55380005606.7Cherepy2009
SrI2SA4.55106; 5115605.28Sturm2011a
SrI2:Ce/NaCe3+4.591600027 (25%); 450 (75%)404; 4356.40.5% Ce/Navanloef2009
SrI2:EuEu2+4.69000012004353.7Cherepy2008
SrI2:EuEu2+4.640000430Hofstadter1968
SrI2:EuEu2+4.59120000120043535% Euvanloef2009
SrI2:EuEu2+4.5511500012004352.86% EuCherepy2009
SrI2:EuEu2+4.55620 (0.5% Eu); 1650 (10% Eu)429 (0.5% Eu); 436 (10% Eu)crystals < 1 cm^3Glodo2010
SrI2:EuEu2+4.55900002.68Sturm2011
SrI2:EuEu2+4.5510400011004322.622.5% Eu2+Rowe2013
SrI2:EuEu2+4.55123; 3,4884302.85Sturm2011a
SrI2:EuEu2+900002.7Sturm2011b
SrI2:YbYb2+4.638400710; 77,000418; 44612.50.5% YbAlekhin2014a
SrI2:YbYb2+4.55560006104144.350.5% Yb2+Rowe2013
Ta2Zn3O8SA7.11130385crystalline powderRack1998
ThBr4SX5.8405Krupa1979
ThCl4SX4.6345Krupa1979
Tl2GdCl5Ce3+5.153,000 ± 5,00032 (76%); 271 (10%); 1600(14%)389~55% Ce in meltKhan2018
Tl2HfCl6SA24,200 (2x1x1 mm)288, 6340450-47017.7Fujimoto2018
Tl2LaCl5Ce3+5.3176,000 (8x6x<1mm)36 (89%); 217(6%); 1500 (11%)3833.43% CeHawrami2017
Tl2LiYCl6:CeCe3+4.5828,000 (1.5 us), 30,000 (4 us), 30,500 (6 us)69 (3%); 459 (84%); 1400 (23%)4304.81% CeKim2016
Tl2LiYCl6:CeCe3+4.52600057 (3%); 431 (64%); 1055 (33%)4354.23% CeHawrami2016
Tl2ZrCl6SA50,800 (2x1x1 mm)696, 2360450-4705.6Fujimoto2018
TlCaCl3Intrinsic3.7730,600 ± 3,060317 (44%); 727 (56%)4255Khan2017
TlCdCl3Tl5.312,200 (1us)2.6 (~8%) 45 (~47%) 170 (~45%)450n/aZeff = 68.7Fujimoto2017
TlCl(Be,I)7100020046542Rosette1970
TlSr2Br5Tl+6.0337600 ± 3700 (6x6x5 mm3 sample)390 (66%); 1900 (34%)4412.4% (2x2x1 mm3); 2.7% (5x8x13 mm3)Rooh2017
TlSr2I5Intrinsic5.331000151 (33%); 605(309); 3000(28%)5288.5Kim2018
TlSr2I5Eu3+5.370000535 (27%); 3300 (73%)4634.23% EuKim2018
Y2O3SX5.04154802837036% of NaI:TlOgorodnikov1996
Y2O3SA5.04930034; 10735018.4Fukabori2010
Y2O3:BiBi3+5410Blasse1968
Y2O3:CeCe3+5Not detectedYen1996
Y2O3:CeCe3+5Not detectedvanderKolk2007
Y2SiO5:Ce (YSO)Ce3+4.459200424209Melcher1996
Y2SiO5:Ce (YSO)Ce3+4.45240009.4Balcerzyk2000b
Y2SiO5:Ce (YSO)Ce3+4.45234000.10% CeCutler2009
Y2SiO5:Ce/Ca (YSO)Ce3+4.45212000.10% Ce; 0.10% CaCutler2009
Y2WO6:BiBi3+1600515Blasse1968
Y3Al5O12:Ce (YAG)SX4.551161010026027% of NaI:TlOgorodnikov1996
Y3Al5O12:Ce (YAG)Ce3+4.5516700Moszynski1997a
Y3Al5O12:Ce (YAG)Ce3+4.553.5Selim2007
Y3Al5O12:Ce (YAG)Ce3+4.55119 + slow300; 550crystal; 0.1% CeMihokova2007
Y3Al5O12:Ce (YAG)Ce3+4.5585 + slow550ceramic; 0.5% CeMihokova2007
Y3Al5O12:PrPr3+6.716000143200.25% PrOgino2006
Y3Al5O12:PrPr3+4.55800018 (80%) + slow300-400Dorenbos1993
YAl3B4O12:BiBi3+3.7290Blasse1968
YAl3B4O12:CeCe3+3.75700344; 367crystalline powderKnitel2000
YAlO3:Ce (YAP)Ce3+5.351620027347Baryshevsky1991
YAlO3:Ce (YAP)Ce3+5.3521600Mares2004
YAlO3:Ce (YAP)Ce3+5.3518000Moszynski1997a
YAlO3:Ce (YAP)Ce3+5.352010024.2365Lempicki1995
YAlO3:Ce (YAP)Ce3+5.3515900deHaas2005
YAlO3:Ce (YAP)Ce3+5.3526 (90%); 67 (10%)risetime: 240 psDerenzo2000
YAlO3:Ce (YAP)Ce3+5.354.4Kapusta1999
YBa3B9O18SA3.9140027400He2007
YBO3:BiBi3+4.51000328Blasse1968
YBO3:CeCe3+4.510000390; 415crystalline powderKnitel2000
YBr3:CeCe3+2000036 (79%); 450 (21%)4221% CeCherginets2012
YCl3:CeCe3+4500390; 4101% Cecherginets2009
YCl3:CeCe3+2.67870037 (86%); 640 (14%)3831% CeCherginets2012
YGd2Ga3Al2O12:CeCe3+4400056.9( 66%); 236 (34%)8.21% CeKamada2011a
YI3:CeCe3+4.698600345492% CeGlodo2008
YMgB5O10:CeCe3+330305crystalline powderKnitel2000
YNb0.2Ta0.8O4SA7.16320(38%); 2,430(62%)440luminosity 6 x YTaO4Voloshyna2014
YNbO4:BiBi3+465Blasse1968
YOBr:CeCe3+61% of ZnS:Ag65405, 440phosphor, 1% CeBuchanan1981
YOBr:CeCe3+5.0610,000*25 (76%); 59 (17%)400; 445* 0.15 x LaBr3:Ce; crystalline powderEagleman2011
YOCl:BiBi3+1400400Blasse1968
YOCl:CeCe3+52% of ZnS:Ag34365, 405phosphor, 1% CeBuchanan1981
YOCl:CeCe3+4.643,500*20 (83%)380* 0.05 x LaBr3:Ce; crystalline powder; 1% CeEagleman2011
YOF:BiBi3+330Blasse1968
YOF:CeCe3+5.23not observedcrystalline powderEagleman2011
YOI:CeCe3+5.425,000*23 (85%)430; 480* 0.07 x LaBr3:Ce; crystalline powder; 1% CeEagleman2011
YPO4:BiBi3+700342Blasse1968
YVO4:BiBi3+4500559Blasse1968
Zn3Ta2O8SA30000270 (18%); 1,060 (80%)385crystalline powderDerenzo2011
ZnO:GaGa3+5.70.36 (35%); 0.82 (65%)fast n-type phosphor, risetime < 40 psDerenzo2000
ZnO:GaGa3+5.7<1385fast n-type phosphorLehmann1966
ZnO:Ga/HGa3+5.797000.8389crystalline powder; luminosity 54% of YAlO3:CeBourret2009
ZnSe:O5.42715004,000; 12,0005957.4luminosity = 1.277 CsI:TlKim2007
ZnSe:TeTe2- BX5.42550005000064513.2Schotanus1992
ZnSe:TeTe2- BX5.42283006105.4Balcerzyk2002
ZnWO4CX7.85930020000Holl1988
ZnWO4CX7.8521800480Grabmaier1984
ZnWO4CX7.85700; 7,000; 25,0008.5Nagornaya2009
ZnWO4CX7.851,000; 4,000; 25,00010.7Kraus2009
ZnWO4CX7.8571702400011.1300KKlamra2012
ZnWO4CX7.8584609.377KKlamra2012